钢渣-杂填土基层材料配合比优化试验研究
作者:
作者单位:

1.安徽工业大学 建筑工程学院,安徽 马鞍山 243032;2.安徽马钢嘉华新型建材有限公司,安徽 马鞍山 243000

作者简介:

黄伟(1963- ),男,教授,主要从事道路材料研究,E-mail:hwpsagd@163.com。
brief:HUANG Wei (1963- ), professor, main research interest: road material, E-mail: hwpsagd@163.com.

通讯作者:

中图分类号:

TU521.3;U414

基金项目:

安徽省高校自然科学研究重大项目(KJ2018ZD006);安徽省住房城乡建设科学技术计划(2018YF-007)


Experimental study on optimization of mix ratio for steel slag-miscellaneous fill base material
Author:
Affiliation:

1.Institute of Civil Engineering, Anhui University of Technology, Maanshan 243032, Anhui, P. R. China;2.Anhui Maanshan Jiahua New Building Materials Co., Ltd., Maanshan 243000, Anhui, P. R. China

Fund Project:

Major Projects of Natural Science Research of Anhui Universities (No. KJ2018ZD006); Anhui Housing Urban and Rural Construction Science and Technology Program Project (No. 2018YF-007)

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    以杂填土、钢渣、矿渣微粉为原料,采用土体固化技术混拌制备钢渣-杂填土基层材料。开展钢渣、混凝土破碎料、素土等主料对基层材料强度的耦合影响试验,构建回归模型,得到主料最优掺入比例,试验验证表明,回归模型预测值误差小于2%;以钢渣、混凝土破碎料、水泥、固化剂为因素开展正交试验,得到的最优结果与强度耦合影响试验基本一致,从而确定钢渣-杂填土最优配合比。最优配合比试件试验结果表明:钢渣-杂填土强度随龄期增长显著提升,30 d高温水浴膨胀率仅为1.03%。X射线衍射分析(XRD)及扫描电子显微镜(SEM)测试表明:矿渣微粉中SiO2与钢渣中f-CaO反应生成水化硅酸钙(C-S-H)凝胶,同时发现土壤固化剂对土体的改性可有效抑制钢渣膨胀;C-S-H凝胶填充于混凝土破碎料、钢渣、土颗粒间,增加了钢渣-杂填土基层材料密实度,使其强度得以提高。

    Abstract:

    Miscellaneous fill, steel slag, and slag powder were mixed to prepare steel slag-miscellaneous fill base material by soil solidification. Firstly, coupling influence test of main materials including steel slag, concrete crushed material and plain soil on the strength of base materials were conducted, regression model was established to obtain optimal mixing ratio. Experimental verification shows that the prediction error was within 2%. Secondly, the orthogonal test was carried out with steel slag, concrete crushing material, cement as well as curing agent as the factors, and the optimal results obtained were basically consistent with the strength coupling influence test. Thus, the optimal mix ratio of steel slag and miscellaneous fill was determined. The test results of the optimal sample showed that the strength increased significantly with age, which presented expansion rate of 1.03% after treatment 30 d high temperature water bath. X-ray diffraction analysis (XRD) and scanning electron microscope (SEM) test results show that SiO2 in slag powder reacted with f-CaO in steel slag to form hydrated calcium silicate gel (C-S-H). It was also confirmed that the modification of the soil solidification agent to the soil can effectively prevent the expansion of steel slag; C-S-H gel is filled in the space of the broken concrete, steel slag as well as soil particles to increase the compactness of the steel slag-miscellaneous fill base material and thus enhance its strength.

    参考文献
    相似文献
    引证文献
引用本文

黄伟,张耄耋,张丽,唐钢,赵鲁卿,王宗森.钢渣-杂填土基层材料配合比优化试验研究[J].土木与环境工程学报(中英文),2022,44(6):12-21. HUANG Wei, ZHANG Maodie, ZHANG Li, TANG Gang, ZHAO Luqing, WANG Zongsen. Experimental study on optimization of mix ratio for steel slag-miscellaneous fill base material[J]. JOURNAL OF CIVIL AND ENVIRONMENTAL ENGINEERING,2022,44(6):12-21.10.11835/j. issn.2096-6717.2021.080

复制
分享
文章指标
  • 点击次数:
  • 下载次数:
  • HTML阅读次数:
  • 引用次数:
历史
  • 收稿日期:2020-10-19
  • 最后修改日期:
  • 录用日期:
  • 在线发布日期: 2022-11-09
  • 出版日期: