Abstract:This paper presents the process of stainless steel ( 1Crl8Ni9Ti) in continuous casting,the components and their shapes,origins and distributions of the large inclusions existing in the steel,as well as the influence on its quality. By the observation through a microscope,the structural analysis adopting x-ray examinating instrument and the measunement for the microzone of billet employing the electronic probe.it has been found that the large inclusions of continuous billet mainly originate from the slag-sweeping of the tundisy and mold. There are mostly spherical-slag in addition to Ti(C.N) in the inclusions. The calculations in theory point out that the siO2in the slag can' t change Ti(C,N) into TiO2,however,it can assimilate with Ti(C.N). The large inclusions affect the quality of the steel plate and tube greatly. As a result,this paper proposes the measures of reducing the large inclusions in the steel.